    Top 5 Common SMT Defects with SAC305 Solder Paste and How to Fix Them

    2026-11-23
    Jufeng Solder

    Troubleshooting SAC305 Solder Paste on the SMT Line

    When an SMT line running SAC305 solder paste (Sn96.5Ag3.0Cu0.5) starts producing defects, first check where the problem appears. Compare the paste deposit after printing with the same location after placement and reflow. That comparison helps narrow down the cause before you change the stencil, the oven settings or the paste.

    Request a TDS or sample Jump to the five defects
    SAC305 solder paste deposits on fine-pitch PCB pads after stencil printing

    Five common SMT defects and where to start

    Use solder paste inspection (SPI) after printing, automated optical inspection (AOI) or microscopy for visible defects, and X-ray for hidden joints such as the thermal pad beneath a QFN.

    1. Solder bridging 2. Insufficient solder 3. Tombstoning 4. Solder balling and mid-chip beads 5. Voiding under QFN thermal pads
    Solder bridge joining two adjacent QFP leads after reflow

    1. Solder bridging

    What you see. Solder joins adjacent pads or leads that should be electrically separate.

    What to check. Look for misaligned, oversized or smeared deposits on SPI or the printer image. If printing is clean, inspect the board after placement for paste squeeze-out and compare the result after reflow.

    How to fix it. Restore stencil-to-board contact, check board support and alignment, and clean the underside of the stencil. For recurring bridges at the same site, review the local apertures and paste volume. If a bridge first appears after reflow, check for hot slump and compare the measured board profile with the paste datasheet.

    How to verify. Confirm that deposits remain separated after printing and the affected leads stay separate after reflow.

    Normal paste deposits on the left and less paste on the center PCB pad on the right

    2. Insufficient solder

    What you see. Too little solder forms at a joint. In severe cases, the joint can be electrically open.

    What to check. Compare SPI volume at the affected pad with the qualified baseline. Check for blocked apertures, inconsistent paste release or reduced volume in the smallest openings.

    How to fix it. Clean the apertures and check squeegee settings and stencil separation. If the same apertures repeatedly release poorly, review the aperture area ratio and stencil thickness. Trial a finer powder grade if the geometry calls for it. If SPI volume is normal, check pad and terminal solderability, lead coplanarity where relevant, and the measured reflow profile.

    How to verify. Confirm stable SPI volume across successive prints and acceptable joints after reflow.

    Tombstoned chip resistor with one end lifted off its PCB pad

    3. Tombstoning

    What you see. One end of a chip resistor or capacitor lifts off its pad as the two ends wet at different times or with unequal force.

    What to check. Compare paste volume and alignment on both pads. Check placement centering and look for unequal copper connections that can make one pad heat faster.

    How to fix it. Center the placement and balance the deposits using the stencil openings. Measure the temperature near both ends on a representative board and reduce the temperature difference within the approved process window. If the defect keeps returning at one footprint, review pad geometry and copper balance.

    How to verify. Check that both ends remain seated and soldered on a trial run covering the affected board positions.

    Scattered solder balls on the left and a solder bead beside a chip resistor on the right

    4. Solder balling and mid-chip beads

    What you see. Fine solder balls may be scattered across the solder mask. A larger bead can appear beside the middle of a chip component.

    What to check. Use the pattern to narrow the cause. For scattered balls, check paste handling, stencil underside smearing, print-to-reflow delay and the heating ramp. For side beads, look for excess paste squeezed under the component body.

    How to fix it. Follow the paste datasheet for storage and working life. Let the sealed container reach working temperature before opening. If paste is spattering, review the measured heating ramp within the approved window. For side beads, correct placement height or force and trial a local aperture shape that keeps paste away from the underside of the chip.

    How to verify. Compare microscope images at the same locations and check that the revised print still produces adequate joints.

    X-ray-style illustration of solder voids beneath a QFN thermal pad

    5. Voiding under QFN thermal pads

    What you see. X-ray shows gaps within the solder joint beneath the exposed pad of a quad flat no-lead (QFN) package.

    What to check. Confirm the void pattern across boards with X-ray. Review the thermal-pad stencil pattern, open vias in the pad and the actual profile at the QFN. These details can affect outgassing and the final solder volume.

    How to fix it. Trial a segmented, windowpane-style stencil opening using the package maker’s coverage guidance. Compare reflow profiles within the approved window. If needed, run a controlled comparison with a lower-voiding paste formulation.

    How to verify. Use the same X-ray settings for the baseline and trial. Evaluate both against the approved criteria for that assembly.

    Confirm the change on a pilot lot

    1. Record the board revision, affected reference designators, paste lot, stencil revision and the last qualified settings.
    2. Save the SPI and AOI images or X-rays for the affected locations. For oven changes, use a thermocouple profile from a representative populated board and compare it with the paste technical data sheet (TDS) and component limits.
    3. Change one variable at a time. Compare the baseline and trial at the same locations and check neighboring joints for new defects before releasing the change.
    View Jufeng SAC305 lead-free solder paste

    Request a SAC305 datasheet or line-trial sample

    Send the component package or minimum pitch, stencil thickness and aperture dimensions, board finish, paste grade, and your defect images or measured reflow profile. For a sample or quote, include the powder grade if known, estimated monthly usage and delivery destination.

    WhatsApp +86 155 7973 7317 marketing002@jufengxi.com Use the Jufeng inquiry form
    Share:

    How to Evaluate SAC305 Solder Paste for Stencil Printing

    Related Article

    image
    Start a SAC305 solder paste stencil printing trial with the smallest apertures on your PCB. Measure deposit volume and variation with solder paste inspection (SPI), then check the first prints after a typical line stop. These results help you decide whether a paste is ready for a production trial.
    How to Evaluate SAC305 Solder Paste for Stencil Printing
    2026-11-20
    image
    A practical look at FC-325LA pressure-assisted silver sintering paste—its printing window, attachment options and recommended processing conditions for large-area bonding.
    Large-Area Silver Sintering: From Stable Printing to Thermal Performance
    2026-10-15
    image
    Copper paste is widely used for via filling in HDI PCBs, TGV substrates, multilayer circuits and advanced electronic packaging. However, one common manufacturing problem is that a via appears completely filled before curing, but becomes recessed, develops voids or loses volume after curing.
    Why Copper Paste Shrinks During Via Filling
    2026-09-22
    image
    Voids in HDI via filling are commonly caused by trapped air, unsuitable paste rheology, incomplete filling, contamination and uncontrolled curing. Reducing them requires the material, via geometry, filling method and curing profile to be evaluated as one complete process.
    How to Reduce Voids in HDI Via Filling
    2026-09-17